A solder bead is a small sphere, typically 0.1–0.5 mm, sitting on the solder mask next to a chip component — often half under the body where AOI struggles to see it. It is routinely confused with splatter, and the two have nothing in common except appearance.
AOI and tilted visual inspection catch beads that hide under chip components
Splatter is random: fine dots scattered across the panel, usually from flux outgassing or moisture, and it does not respect component boundaries. Beading is local: it clusters around specific components, is roughly spherical, and is metallic rather than flux residue.
The mechanism explains the shape. Paste that has been displaced off the pad has no wettable surface to spread on. At reflow it coalesces into a sphere under surface tension and stays there, sitting on mask that solder cannot wet. So the question is always: what pushed that paste off the pad?
This is the most common cause on 0402 and 0201. The nozzle seats the part and squeezes paste out from under both terminations. The squeezed paste lands beside the pad and balls up. The pattern is a bead on one or both sides of a specific component type, repeated at the same orientation.
Reduce placement force to the minimum that seats the part, recalibrate Z-offset for the actual board thickness, and check the nozzle for wear. On 0201 the working window is tens of microns, so "it worked on the last board" is not evidence.
When the stencil does not seal — low tension, insufficient support, panel warp, a worn aperture edge — paste is pressed under the stencil around the aperture. After separation it leaves a thin ring of paste on the mask beside the pad, which becomes a bead at reflow.
Signature: beads arranged around many apertures in one region, plus a faint halo of paste visible on the mask before reflow. Check the stencil underside after a print; if there is paste where there should be none, this is the cause.
Paste with too much solvent, or paste heated too quickly, loses shape before coalescence. The deposit slumps sideways, a fillet of paste reaches the mask, and it balls up independently. Look for beads on the side of the component facing a hot zone or a large copper area, and for a ramp above 2–3 °C/s.
Paste handling matters as much as the profile: warm to room temperature before opening (typically two hours for a syringe or jar), stay inside the open time, keep 23 ± 3 °C and 40–60% RH, and never top up old paste with new.
Paste transferred to the underside during wiping is pressed onto the next board and appears as beads in a pattern that shifts between panels. If the beads move, suspect the wipe: dry wipe every 3–5 prints, solvent wipe at a longer interval, and a vacuum under-stencil wipe rather than a dry cloth alone.
Via-in-pad without plugging wicks paste into the barrel; the remainder reflows as a bead at the via edge. Openings in the mask near a pad give the paste somewhere to flow. Both are design issues caught at DFM, not process issues.
A bead under a chip body is invisible to a top-down camera. Use tilted AOI cameras where available, add a visual inspection step at the reflow exit for high-reliability builds, and remember the acceptance criterion is electrical, not cosmetic: a bead is a defect when it reduces clearance below the specification or sits between two conductors.
For automotive and medical builds we treat beads adjacent to fine-pitch parts as a defect regardless of clearance, because vibration and coating can move the failure later.
Most lines that "have a beading problem" actually have two: a placement setting and a wipe interval. Fix the placement first, because it is deterministic; then tighten the wipe schedule and re-measure over a full shift rather than a single panel.